Nov. 2026 | Dr. Noh Chang-ho (Senior Analyst), UBI Research
5. Native RGB Single-Junction Micro OLED: INT-Tech and Guanyu
Taiwan’s INT-Tech and China’s Taizhou Guanyu Technology presented paper 44-2, “150,000nits Full-color Native RGB Single Junction 3,386PPI Micro-OLED,” at SID Display Week in May 2026. The 0.39-inch XGA (1024×768) panel was made with uNEEDXR, a process system developed over nine years that integrates design, process, equipment, and materials; on a 0.18 µm CMOS backplane, a single-junction RGB device with a 7.5 µm pixel pitch (3,386 ppi) reached a measured maximum luminance of 151,605 nits (Table 5, Figure 5). INT-Tech had unveiled a 100,000-nit product of the same size in December 2025. The paper gives two sets of subpixel values: a diameter of 3.5 µm with a 51% aperture ratio (Methods) and 3.3 µm with 58% (Results).
The process begins by patterning the anode and pixel-defining layer (PDL) on an 8-inch wafer and depositing common HIL and HTL layers through an open metal mask. Then, in an environment shielded from oxygen and moisture, only the pixel areas of the first color are selectively exposed, and the emitting layer and ETL of that color are deposited; the same steps are repeated to form the second and third colors. The cathode is deposited over the entire surface with an open mask, and the device is encapsulated with TFE and vacuum lamination of a cover glass. All organic materials are commercial materials. The paper cites clogging and alignment issues of ultra-fine mask methods and plasma and moisture damage of dry and wet etching methods as limitations of existing technologies.
Compared with a commercial 0.39-inch XGA W-OLED+CF product of the same size, the paper reports one-fifth the power consumption at 3,000 nits, 11 times the luminance at the same power of 550 mW, and more than five times lower current density at the same luminance. The color gamut is 95% of DCI-P3, wider than W-OLED+CF (about 81%). Lifetime is described only as meeting customers’ reliability and lifetime requirements, without figures. Compared with SEL’s MML tandem device in Section 4 (3,207 ppi, 15,000 nits), the pixel density is similar and the luminance is ten times higher.
Table 5. INT-Tech/Guanyu 0.39-inch native RGB micro-OLED (SID 2026)
Item | Specification |
Panel | 0.39", XGA (1024×RGB×768), 0.18 µm CMOS backplane |
Pixel density | 3,386 ppi (pixel pitch 7.5 µm), single junction, no color filter |
Max luminance | 150,000 nits ±5% at 9 V (measured 151,605 nits) |
Power | <3,000 mW at 150,000 nits; 1/5 of W-OLED+CF at 3,000 nits |
Contrast ratio | >100,000:1 at 150,000 nits |
Color | DCI-P3 95%; peaks R 625 / G 525 / B 463 nm; FWHM <36 nm |
Uniformity | >90% (nine-point average) |
Source: K.-C. Hsu et al., SID 2026 Digest, 44-2 (INT-Tech, Taizhou Guanyu Technology)

Figure 5. INT-Tech native RGB 0.39-inch panel and RGB pixel array (7.5 µm pitch)
Source: K.-C. Hsu et al., SID 2026 Digest, 44-2, Figure 3
6. Direct Patterning of Emitting Materials: ETH Zurich
On September 16, 2026, a research team led by Professor Chih-Jen Shih of ETH Zurich and Professor Yinyin Bao of the University of Helsinki reported in Nature an electroluminescent photoresist (ELPR), in which the emitting-layer material also serves as the photoresist (Nature vol. 658, October 1 issue). A TADF emitter sits at the core of a star-shaped polymer synthesized by atom transfer radical polymerization (ATRP), and each arm consists of a phenylcarbazole-based host block and an outer cross-linking block, so that cross-linking occurs only at molecular boundaries. Exposed areas are cross-linked and unexposed areas are removed with toluene; because the cross-linked pattern does not dissolve in the developer for the next color, exposure can be repeated for each color. It differs from the MML method in Section 4 in that it patterns the emitting layer directly, without a sacrificial layer or etching. The authors have filed a European patent application on the ELPR concept and synthesis method (EP25223816.7).
Patterning resolution is L/S 4/2 µm with 365 nm UV exposure and L/S 110/160 nm with electron-beam exposure. In electrically driven devices, the green self-host polymer reached a maximum EQE of 30.3%, higher than an evaporated control device with the same emitter (26.5%), and ELPR that also underwent UV cross-linking recorded 13.3% for green and 10.4% for red. The EQE of earlier photopatternable emitting polymers was generally below 2%. In a multicolor demonstration, three rounds of lithography on an ITO/SiO2 structure on a glass substrate produced the letters “ETH” with 30 µm pixels, driven at 6 V (Figure 6).

Figure 6. ELPR three-colour OLED: device structure (e) and 30 µm 'ETH' pixels (f, g)
Source: Lo et al., Nature 658, 78 (2026), Fig. 5e–g, CC BY 4.0
The challenges are lifetime and pixel size. Even after residual copper from the catalyst was halved by dialysis, LT50 at 2.4 mA/cm² was 146 minutes for cross-linked ELPR and 172 minutes for the polymer, and continuous operation is limited to 10 mA/cm² or less. The authors proposed reducing copper with regenerative or organocatalyzed ATRP.
7. Comparison of Approaches and Subpixel Isolation Patents
The three routes differ in what determines the pattern size (Table 6, Figure 7). Mask evaporation uses existing vacuum evaporation lines and materials as they are, and a mass-production schedule has been announced. In photolithography and direct patterning of emitting materials, the exposure tool determines the pattern size, giving a large resolution margin, but process damage to organic films and lifetime remain challenges.
Table 6. Three approaches to Direct RGB OLEDoS patterning
Item | Shadow-mask evaporation | Photolithography | Photopatternable emitter |
Pitch set by | Mask opening and alignment | Lithography tool | Lithography tool |
Emitter | Evaporated small molecule | Evaporated small molecule | Cross-linkable polymer |
Players | Samsung Display, Canon Tokki, Sunic System | SEL, Ruixian, Visionox (glass) | ETH Zurich |
Best result | 5,000 ppi (Samsung Display) | 3,207 ppi, 15,000 nits (SEL) | 110 nm (EBL, PL); 30 µm EL pixels (ETH) |
Main issue | Shadow, mask sag, mask cost | Process damage, step count | Lifetime |
Production plan | Samsung Display from 2028 | Not announced | 5–10 years (authors) |
Source: Company announcements, CN 122959660 A, ETH Zurich; compiled by UBI Research

Figure 7. Patterning routes for Direct RGB OLEDoS by company
In tandem RGB for high luminance, when the subpixel spacing narrows to a few µm, lateral leakage through common layers such as the charge generation layer (CGL) causes color mixing. This issue applies to both the mask and photolithography routes. Over the past year, Samsung Display published a structure in which an undercut separation wall formed by etch-back cuts the CGL (US 2026/0282632 A1), and BOE and its subsidiary Yunnan Invensight (云南创视界) published a separation structure that expands when heated after deposition to block adjacent devices (CN224069067U, utility model). SEL’s US 12,787,587 B2 also covers the etched side faces of the EL layer with an insulating layer.
8. Outlook
Direct RGB OLEDoS is divided into mask evaporation ahead of mass production in 2028 (Samsung Display, Canon Tokki, Sunic System), photolithography accumulating granted patents (SEL, Ruixian), and direct patterning of emitting materials at the academic stage (ETH Zurich). INT-Tech (Guanyu) presented a 150,000-nit single-junction prototype. If Samsung Display’s schedule holds, the first mass production of RGB OLEDoS will start in 2028 with FSM-based mask evaporation (Figure 8). Canon Tokki’s ±0.04 µm-class alignment and Sunic System’s 0.15 µm-class RGB equipment specification indicate that equipment precision has approached the level required for separate RGB evaporation. The remaining variables are the supply and cost of masks with openings of a few µm.

Figure 8. Key events and planned milestones for Direct RGB OLEDoS
Noh Chang-ho, chnoh@ubiresearch.com